抄録
The sludge deposition of JIS die casting alloy ADC12 in the holding furnace was studied. A quaternary intermetallic compound (FeMn)3Si2Al15 deposits in the molten metal free from Cr. Critical Fe and Mn concentrations for sludge deposition at a holding temperature T°C are expressed as: %Fe+{3.34-(T-630)/714}%Mn = 2.39+(T-630)/152 A quinary Al-Si-Fe-Mn-Cr compound (FeMnCr) 3Si2Al15 deposits in the molten metal containing Cr. Critical concentrations of Mn and Cr in molten ADC12 alloys containing 1.0% of Fe at a temperature T°C are expressed as: %Mn+{4.00+(T-630)/333}%Cr=0.40+(T-630)/500.
本文言語 | English |
---|---|
ページ(範囲) | 813-818 |
ページ数 | 6 |
ジャーナル | Journal of Japan Institute of Light Metals |
巻 | 36 |
号 | 12 |
DOI | |
出版ステータス | Published - 1986 |
外部発表 | はい |
ASJC Scopus subject areas
- 材料力学
- 機械工学
- 金属および合金
- 材料化学